1.4301 is the European material number for the stainless steel that most US engineers simply call Type 304 (UNS S30400). Its EN steel name is X5CrNi18-10: an austenitic chromium-nickel grade with no molybdenum and the workhorse of the stainless industry. When a European drawing quotes 1.4301, read it as 304 for most practical purposes; the limits, however, come from EN standards, not ASTM. This page covers chemistry, minimum mechanical properties in MPa and ksi, physical data, corrosion and temperature limits, welding notes, and the 304 pipe, bar, sheet, flange and elbow categories we ship from the EU (Poland).
Chemical composition of 1.4301 (wt. %)
| C | Si | Mn | Cr | Ni | N |
|---|---|---|---|---|---|
| ≤ 0.07 | ≤ 1.00 | ≤ 2.00 | 17.5–19.5 | 8.0–10.5 | ≤ 0.10 |
Limits per EN 10088. They are very close to the ASTM limits for Type 304 but not identical word for word. The actual heat analysis is stated on the EN 10204 3.1 inspection certificate, available on request.
Mechanical properties of 1.4301 – yield and tensile strength
| Property | Bar (EN 10088-3) | Seamless pipe (EN 10216-5) | Cold-rolled sheet (EN 10088-2) |
|---|---|---|---|
| Yield strength Rp0.2 [MPa] | ≥ 190 (28 ksi) | ≥ 210 (30 ksi) | ≥ 230 (33 ksi) |
| Tensile strength Rm [MPa] | 500–700 (73–102 ksi) | 520–720 (75–104 ksi) | 540–750 (78–109 ksi) |
| Elongation A [%] | ≥ 45 | ≥ 45 | ≥ 45 |
| Hardness | ≤ 215 HB | ≤ 215 HB | ≤ 215 HB |
Minimum or range values in the solution-annealed condition; ksi figures are rounded conversions. Actual properties depend on product form and size (diameter or wall/plate thickness). The binding values for your material are those on the EN 10204 3.1 inspection certificate, available on request.
Physical properties
| Property | Value |
|---|---|
| Density | 7.9 g/cm³ (approx. 0.285 lb/in³) |
| Modulus of elasticity | 200 GPa (approx. 29,000 ksi) |
| Thermal conductivity | 15 W/(m·K) (approx. 8.7 BTU/(h·ft·°F)) |
| Magnetic behavior | practically non-magnetic when solution annealed; slightly magnetic after cold working |
What is 1.4301 in US terms? AISI, UNS and ASTM
| EN number | EN steel name | AISI / Type | UNS |
|---|---|---|---|
| 1.4301 | X5CrNi18-10 | Type 304 | S30400 |
For comparison only: in US practice Type 304 pipe is usually ordered to ASTM A312, tubing to ASTM A269 or A213, bar to ASTM A276 or A479, and plate, sheet and strip to ASTM A240. Our material is produced to EN standards; the ASTM numbers are reference points only, not a claim of ASTM certification. Pipe is described by outside diameter and wall thickness in mm rather than by NPS and Schedule, so convert your nominal size before you compare.
Corrosion resistance and PREN of Type 304
Chromium forms a thin passive film on the surface that repairs itself in air after scratching. As a result, Type 304 resists water, steam, humidity, most foods and many organic and weak inorganic acids. Its pitting resistance equivalent number (PREN) is roughly 18–20. Because 304 contains no molybdenum, it is the wrong choice where chlorides are present – seawater, indoor pool air, or deicing salt splashed from roads in winter. For those conditions, specify 1.4404 (316L) or 1.4571 (316Ti).
Maximum service temperature
In continuous service 1.4301 can be used up to about 300 °C (approx. 570 °F) without restrictions. Scaling resistance in air reaches about 850 °C (approx. 1560 °F), but 304 is not a heat-resistant grade in the EN 10095 sense. For sustained high temperatures look at titanium-stabilized 1.4541 (Type 321) or the heat-resistant 1.4841 (Type 314).
Welding and fabrication
Type 304 welds very well with every common process – GTAW (TIG), GMAW (MIG) and SMAW (stick). On heavy-wall parts that will not be solution annealed after welding, the low-carbon 1.4307 (304L) is the safer choice against intergranular corrosion in the heat-affected zone. The grade cold forms easily; cold work increases strength and can make it slightly magnetic. Like every austenitic stainless it work-hardens during machining, so use sharp tools and a steady feed. Pickle away heat tint color after welding.
Typical applications
- Food processing, dairy and brewery equipment
- Household appliances
- Interior architecture and trim
- Structural parts, tanks and vessels
- Piping for water and chloride-free process media
304 vs 304L vs 316L
1.4307 (304L) caps carbon at C ≤ 0.030 % and holds up better after welding thick sections. 1.4306 is also a 304L-type grade, with higher nickel. A lot of material on the market is dual-certified 304/304L (1.4301/1.4307), meaning one heat satisfies both sets of limits – which is why our category names read 304/304L. 1.4404 (316L) adds molybdenum and copes far better with chlorides.
Type 304 products from Stainless Europe
Shop 1.4301 / Type 304 by product form:
- 304/304L Stainless Steel Seamless Pipe & Tube
- 304/304L Stainless Steel Round Bar
- 304 Stainless Steel Sheet
- 304/304L Stainless Steel Flanges
- 304/304L Stainless Steel Elbows
Every order can be supplied with an EN 10204 3.1 inspection certificate on request. We ship from the EU (Poland).
FAQ: 1.4301 / Type 304
Is 1.4301 the same as 304?
For practical purposes, yes. 1.4301 (X5CrNi18-10) is the EN counterpart of Type 304 / UNS S30400. The limits are defined in EN 10088 rather than ASTM, so check the certificate if your job requires ASTM compliance.
Is 304 stainless steel magnetic?
In the solution-annealed condition it is practically non-magnetic. After cold working (bending, drawing, forming) it can become slightly magnetic; this does not reduce corrosion resistance.
What is the difference between 304 and 304L?
304L (1.4307) limits carbon to C ≤ 0.030 %, which protects welded heavy sections against intergranular corrosion. Dual-certified 304/304L meets both specifications.
Can 304 stainless be used in saltwater?
It is not recommended. Without molybdenum, 304 is prone to pitting in chloride environments. Use 316L (1.4404) instead.
What is the maximum temperature for 304?
Up to about 300 °C (approx. 570 °F) in continuous service without restrictions; scaling resistance in air up to about 850 °C (approx. 1560 °F). For higher temperatures choose a heat-resistant grade.